Aluminium · Aluminium extrusions · isotropic

EN AW-7020 T6

EN 1999-1-1 · extrusions and drawn tube · buckling class A

EN AW-7020 T6 is an aluminium alloy and temper for extrusions to EN 1999-1-1. Its characteristic 0.2 % proof strength is 275–290 MPa, depending on the product form and thickness. E = 70 GPa, ν = 0.3 and α = 23 × 10⁻⁶/K (design values).

Record
al-7020-t6-ext
Library
v1.1.0
Properties
9
Sources
1
Build check
passed ✓
Viewing as
guest
+ Compare Cite Download · PRO
E · Young's modulus 70GPa design[1]
ν · Poisson's ratio 0.3– design[1]
f_o · 0.2 % proof strength 290MPa char[1]EP, ET, ER/B · t ≤ 15 mm
f_u · Tensile strength (R_m) 350MPa char[1]EP, ET, ER/B · t ≤ 15 mm
ρ · Density 2700kg/m³ design[1]
α · Coefficient of thermal expansion 2310⁻⁶/K design[1]

Elastic constants

isotropic
SymbolPropertyValueUnitBasisRef.
E Young's modulus ⓘ EN 1999-1-1 3.2.5 70 GPa design [1]
G Shear modulus 27 GPa design [1]
ν Poisson's ratio 0.3 – design [1]
K Bulk modulus K = E / 3(1 − 2ν) 58.33 GPa derived —
λ_L Lamé constant λ_L = Eν / (1 + ν)(1 − 2ν) 40.38 GPa derived —
c₀ Bar wave speed c₀ = √(E/ρ) 5092 m/s derived —

Physical, thermal and electrical

at 20 °C
SymbolPropertyValueUnitBasisRef.
α Coefficient of thermal expansion ⓘ for T < 100 °C 23 10⁻⁶/K design [1]
ρ Density 2700 kg/m³ design [1]

Strength

a band applies up to and including its upper limit
PropertyProduct formThicknessValueUnitBasisRef.
f_oEP, ET, ER/B — EP, ET, ER/Bt ≤ 15 mm290MPachar[1]
f_oEP, ET, ER/B — EP, ET, ER/Bt ≤ 40 mm275MPachar[1]
f_oDT — drawn tubet ≤ 20 mm280MPachar[1]
f_uEP, ET, ER/B — EP, ET, ER/Bt ≤ 15 mm350MPachar[1]
f_uEP, ET, ER/B — EP, ET, ER/Bt ≤ 40 mm350MPachar[1]
f_uDT — drawn tubet ≤ 20 mm350MPachar[1]
SymbolPropertyValue at t = 15 mm · EP, ET, ER/BUnitBasisRef.
f_o 0.2 % proof strength ⓘ thickness is the upper limit of each row 290 MPa char [1]
f_u Tensile strength (R_m) 350 MPa char [1]
f_o,haz 0.2 % proof strength in the heat-affected zone ⓘ MIG welding; EN 1999-1-1 reduces HAZ values for TIG and thicker parts 205 MPa char [1]
f_u,haz Tensile strength in the heat-affected zone 280 MPa char [1]

Sources

every value names one
  1. EN 1999-1-1:2007, Eurocode 9 — Design of aluminium structures, Table 3.2b and 3.2.5Copies checked: 1, 2, 3, 4

min product standard minimum char characteristic design code value for design typical datasheet or textbook derived worked out here, formula shown

Cite this page

for reports and papers

BadgerMecX Materials (2026). EN AW-7020 T6 — material properties, EN 1999-1-1. Library v1.1.0, record al-7020-t6-ext. https://staging.badgermecx.com/materials/al-7020-t6-ext/ (accessed 2026-11-26).

@misc{badgermecx_al7020t6ext,
  title  = {EN AW-7020 T6 -- material properties, EN 1999-1-1},
  author = {{BadgerMecX Materials}},
  year   = {2026},
  note   = {Library v1.1.0, record al-7020-t6-ext},
  url    = {https://staging.badgermecx.com/materials/al-7020-t6-ext/}
}

Export and related

SI units, every value with basis and source