Composite · UD lamina, carbon · orthotropic
AS4/3501-6 carbon/epoxy
Herakovich (1998) · V_f = 0.62
AS4/3501-6 carbon/epoxy is a unidirectional carbon-fibre lamina to Herakovich (1998). Along the fibres E₁ = 148 GPa; across them E₂ = 10.5 GPa.
- Record
- ud-as4-3501-6
- Library
- v1.1.0
- Properties
- 11
- Sources
- 1
- Build check
- passed ✓
- Viewing as
- guest
Elastic constants
orthotropic| Symbol | Property | Value | Unit | Basis | Ref. |
|---|---|---|---|---|---|
| E₁ | Modulus, direction 1 | 148 | GPa | typical | [1] |
| E₂ | Modulus, direction 2 | 10.5 | GPa | typical | [1] |
| E₃ | Modulus, direction 3 ⓘ transverse isotropy: E₃ = E₂ | 10.5 | GPa | derived | [1] |
| ν₁₂ | Poisson's ratio 1-2 ⓘ the major Poisson's ratio (printed as ν₂₁ in the copy checked) | 0.3 | – | typical | [1] |
| ν₁₃ | Poisson's ratio 1-3 ⓘ transverse isotropy: ν₁₃ = ν₁₂ | 0.3 | – | derived | [1] |
| ν₂₃ | Poisson's ratio 2-3 | 0.59 | – | typical | [1] |
| G₁₂ | Shear modulus 1-2 | 5.61 | GPa | typical | [1] |
| G₁₃ | Shear modulus 1-3 ⓘ transverse isotropy: G₁₃ = G₁₂ | 5.61 | GPa | derived | [1] |
| G₂₃ | Shear modulus 2-3 | 3.17 | GPa | typical | [1] |
Stiffness matrix C [GPa] · Voigt order 11, 22, 33, 23, 13, 12
| 152.8 | 7.93 | 7.93 | 0 | 0 | 0 |
| 7.93 | 16.52 | 9.915 | 0 | 0 | 0 |
| 7.93 | 9.915 | 16.52 | 0 | 0 | 0 |
| 0 | 0 | 0 | 3.17 | 0 | 0 |
| 0 | 0 | 0 | 0 | 5.61 | 0 |
| 0 | 0 | 0 | 0 | 0 | 5.61 |
C = S⁻¹ from the engineering constants above; checked positive definite when the library is built.
Physical, thermal and electrical
at 20 °CNotes
- Full 3D constants. The printed G₂₃ is not exactly E₂/(2(1 + ν₂₃)) = 3302 MPa, as strict transverse isotropy would require; the record keeps the printed value.
Sources
every value names one- C. T. Herakovich, Mechanics of Fibrous Composites (1998), p. 245 — as tabulated in Johnson, Aerospace Structures, Table 8.2Copies checked: 1
min product standard minimum char characteristic design code value for design typical datasheet or textbook derived worked out here, formula shown
Cite this page
for reports and papersBadgerMecX Materials (2026). AS4/3501-6 carbon/epoxy — material properties, Herakovich (1998). Library v1.1.0, record ud-as4-3501-6. https://staging.badgermecx.com/materials/ud-as4-3501-6/ (accessed 2026-11-26).
@misc{badgermecx_udas435016,
title = {AS4/3501-6 carbon/epoxy -- material properties, Herakovich (1998)},
author = {{BadgerMecX Materials}},
year = {2026},
note = {Library v1.1.0, record ud-as4-3501-6},
url = {https://staging.badgermecx.com/materials/ud-as4-3501-6/}
}