Steel · Structural steel · isotropic

S355

EN 10025-2 · hot rolled, non-alloy

S355 is a structural steel to EN 10025-2. Its minimum yield strength is 355 MPa up to 16 mm thick and falls in steps to 295 MPa at 100–150 mm. E = 210 GPa, ν = 0.3 and α = 12 × 10⁻⁶/K (design values).

Record
steel-s355
Library
v1.1.0
Properties
12
Sources
5
Build check
passed ✓
Viewing as
guest
+ Compare Cite Download · PRO
E · Young's modulus 210GPa design[1]
ν · Poisson's ratio 0.3– design[1]
f_y · Yield strength (R_eH / R_p0.2) 355MPa min[2]t ≤ 16 mm
f_u · Tensile strength (R_m) 470MPa min[2]t ≤ 100 mm
ρ · Density 7850kg/m³ design[3]
α · Coefficient of thermal expansion 1210⁻⁶/K design[1]
λ · Thermal conductivity 53.33W/(m·K) derived[3]
c_p · Specific heat capacity 439.8J/(kg·K) derived[3]

Elastic constants

isotropic
SymbolPropertyValueUnitBasisRef.
E Young's modulus 210 GPa design [1]
G Shear modulus ⓘ EN 1993-1-1 3.2.6: G = E/(2(1 + ν)) ≈ 81 000 MPa 81 GPa design [1]
ν Poisson's ratio 0.3 – design [1]
K Bulk modulus K = E / 3(1 − 2ν) 175 GPa derived —
λ_L Lamé constant λ_L = Eν / (1 + ν)(1 − 2ν) 121.2 GPa derived —
c₀ Bar wave speed c₀ = √(E/ρ) 5172 m/s derived —

Physical, thermal and electrical

at 20 °C
SymbolPropertyValueUnitBasisRef.
α Coefficient of thermal expansion ⓘ up to 100 °C 12 10⁻⁶/K design [1]
ρ Density ⓘ independent of temperature (EN 1993-1-2 3.2.2) 7850 kg/m³ design [3]
λ Thermal conductivity ⓘ λ_a = 54 − 3.33×10⁻²·θ at θ = 20 °C 53.33 W/(m·K) derived [3]
c_p Specific heat capacity ⓘ c_a = 425 + 0.773θ − 1.69×10⁻³θ² + 2.22×10⁻⁶θ³ at θ = 20 °C 439.8 J/(kg·K) derived [3]
a Thermal diffusivity a = λ / (ρ·c_p) 15.45 mm²/s derived —

Strength

a band applies up to and including its upper limit
16406380100150 280300320340360380
f_y [MPa] · t [mm]
Propertyt ≤ 1616–4040–6363–8080–100100–150BasisRef.
f_y Yield strength (R_eH / R_p0.2) MPa355345335325315295min[2]
f_u Tensile strength (R_m) MPa470470470470470450min[2]
f_u,max Tensile strength, upper limit MPa630630630630630600min[2]
f_y (T3.1) Yield strength, EN 1993-1-1 Table 3.1 MPa355355335335——nominal[1]
f_u (T3.1) Tensile strength, EN 1993-1-1 Table 3.1 MPa490490470470——nominal[1]
SymbolPropertyValue at t = 16 mmUnitBasisRef.
f_y Yield strength (R_eH / R_p0.2) ⓘ R_eH, minimum, by nominal thickness 355 MPa min [2]
f_u Tensile strength (R_m) ⓘ R_m lower limit; the 100 mm band starts at 3 mm 470 MPa min [2]
f_u,max Tensile strength, upper limit ⓘ R_m upper limit of the range 630 MPa min [2]
f_y (T3.1) Yield strength, EN 1993-1-1 Table 3.1 355 MPa nominal [1]
f_u (T3.1) Tensile strength, EN 1993-1-1 Table 3.1 490 MPa nominal [1]

Properties against temperature

20–1200 °C

Sign in with a free account to see this section.

Sign in

Nonlinear material models

for FE analysis

Sign in with a free account to see this section.

Sign in

Fatigue strength curves

direct stress ranges

Sign in with a free account to see this section.

Sign in

Notes

  • EN 1993-1-1 3.2.1 lets the design take f_y = R_eH and f_u = R_m,min from EN 10025-2, or the simplified values of its Table 3.1; the National Annex may choose.

Sources

every value names one
  1. EN 1993-1-1:2005, Eurocode 3 — Design of steel structures — General rules, 3.2.6 and Table 3.1Copies checked: 1
  2. EN 10025-2:2019, Hot rolled products of structural steels — Part 2: non-alloy structural steelsCopies checked: 1
  3. EN 1993-1-2:2005, Eurocode 3 — Structural fire design, 3.2.1 (Table 3.1), 3.2.2 (Figure 3.1) and 3.4.1 (thermal properties of steel)Copies checked: 1, 2, 3

min product standard minimum char characteristic design code value for design typical datasheet or textbook derived worked out here, formula shown

Cite this page

for reports and papers

BadgerMecX Materials (2026). S355 — material properties, EN 10025-2. Library v1.1.0, record steel-s355. https://staging.badgermecx.com/materials/steel-s355/ (accessed 2026-11-26).

@misc{badgermecx_steels355,
  title  = {S355 -- material properties, EN 10025-2},
  author = {{BadgerMecX Materials}},
  year   = {2026},
  note   = {Library v1.1.0, record steel-s355},
  url    = {https://staging.badgermecx.com/materials/steel-s355/}
}

Export and related

SI units, every value with basis and source