Timber · Solid timber, hardwood · orthotropic
D30
EN 338:2016 · strength class, 12 % moisture reference
D30 is a hardwood strength class to EN 338:2016. Its characteristic bending strength is 30 MPa. Along the fibres E₁ = 11 GPa; across them E₂ = 0.73 GPa.
- Record
- timber-d30
- Library
- v1.1.0
- Properties
- 14
- Sources
- 1
- Build check
- passed ✓
- Viewing as
- guest
Elastic constants
orthotropic| Symbol | Property | Value | Unit | Basis | Ref. |
|---|---|---|---|---|---|
| E₁ | Modulus, direction 1 ⓘ E_0,mean, along the grain | 11 | GPa | mean | [1] |
| E₀,₀₅ | Modulus parallel to grain, 5 % fractile | 9.2 | GPa | char | [1] |
| E₂ | Modulus, direction 2 ⓘ E_90,mean, across the grain | 0.73 | GPa | mean | [1] |
| E₃ | Modulus, direction 3 ⓘ E_90,mean — the standard does not separate radial and tangential | 0.73 | GPa | mean | [1] |
| G₁₂ | Shear modulus 1-2 ⓘ G_mean | 0.69 | GPa | mean | [1] |
| G₁₃ | Shear modulus 1-3 ⓘ G_mean | 0.69 | GPa | mean | [1] |
Physical, thermal and electrical
at 20 °CStrength
a band applies up to and including its upper limit| Symbol | Property | Value | Unit | Basis | Ref. |
|---|---|---|---|---|---|
| f_m,k | Bending strength | 30 | MPa | char | [1] |
| f_t,0,k | Tension parallel to grain | 18 | MPa | char | [1] |
| f_t,90,k | Tension perpendicular to grain | 0.6 | MPa | char | [1] |
| f_c,0,k | Compression parallel to grain | 24 | MPa | char | [1] |
| f_c,90,k | Compression perpendicular to grain | 5.3 | MPa | char | [1] |
| f_v,k | Shear strength | 3.9 | MPa | char | [1] |
Notes
- EN 338 and EN 14080 give no Poisson's ratios; a 3D analysis needs them from another source.
Sources
every value names onemin product standard minimum char characteristic design code value for design typical datasheet or textbook derived worked out here, formula shown
Cite this page
for reports and papersBadgerMecX Materials (2026). D30 — material properties, EN 338:2016. Library v1.1.0, record timber-d30. https://staging.badgermecx.com/materials/timber-d30/ (accessed 2026-11-26).
@misc{badgermecx_timberd30,
title = {D30 -- material properties, EN 338:2016},
author = {{BadgerMecX Materials}},
year = {2026},
note = {Library v1.1.0, record timber-d30},
url = {https://staging.badgermecx.com/materials/timber-d30/}
}