Timber · Glued laminated timber, homogeneous · orthotropic
GL32h
EN 14080:2013 · strength class
GL32h is a homogeneous glued laminated timber class to EN 14080:2013. Its characteristic bending strength is 32 MPa. Along the fibres E₁ = 14.2 GPa; across them E₂ = 0.3 GPa.
- Record
- glulam-gl32h
- Library
- v1.1.0
- Properties
- 19
- Sources
- 1
- Build check
- passed ✓
- Viewing as
- guest
Elastic constants
orthotropic| Symbol | Property | Value | Unit | Basis | Ref. |
|---|---|---|---|---|---|
| E₁ | Modulus, direction 1 ⓘ E_0,g,mean | 14.2 | GPa | mean | [1] |
| E₀,₀₅ | Modulus parallel to grain, 5 % fractile | 11.8 | GPa | char | [1] |
| E₂ | Modulus, direction 2 ⓘ E_90,g,mean | 0.3 | GPa | mean | [1] |
| E₃ | Modulus, direction 3 ⓘ E_90,g,mean | 0.3 | GPa | mean | [1] |
| G₁₂ | Shear modulus 1-2 ⓘ G_g,mean | 0.65 | GPa | mean | [1] |
| G₁₃ | Shear modulus 1-3 ⓘ G_g,mean | 0.65 | GPa | mean | [1] |
| G₀₅ | Shear modulus, 5 % fractile | 0.54 | GPa | char | [1] |
| E₉₀,₀₅ | Modulus perpendicular to grain, 5 % fractile | 0.25 | GPa | char | [1] |
| G₂₃ | Shear modulus 2-3 ⓘ G_r,g,mean, rolling shear | 0.065 | GPa | mean | [1] |
| G_r | Rolling shear modulus | 0.065 | GPa | mean | [1] |
Physical, thermal and electrical
at 20 °CStrength
a band applies up to and including its upper limit| Symbol | Property | Value | Unit | Basis | Ref. |
|---|---|---|---|---|---|
| f_m,k | Bending strength | 32 | MPa | char | [1] |
| f_t,0,k | Tension parallel to grain | 25.6 | MPa | char | [1] |
| f_t,90,k | Tension perpendicular to grain | 0.5 | MPa | char | [1] |
| f_c,90,k | Compression perpendicular to grain | 2.5 | MPa | char | [1] |
| f_v,k | Shear strength | 3.5 | MPa | char | [1] |
| f_c,0,k | Compression parallel to grain | 32 | MPa | char | [1] |
| f_r,k | Rolling shear strength | 1.2 | MPa | char | [1] |
Notes
- EN 338 and EN 14080 give no Poisson's ratios; a 3D analysis needs them from another source.
Sources
every value names onemin product standard minimum char characteristic design code value for design typical datasheet or textbook derived worked out here, formula shown
Cite this page
for reports and papersBadgerMecX Materials (2026). GL32h — material properties, EN 14080:2013. Library v1.1.0, record glulam-gl32h. https://staging.badgermecx.com/materials/glulam-gl32h/ (accessed 2026-11-26).
@misc{badgermecx_glulamgl32h,
title = {GL32h -- material properties, EN 14080:2013},
author = {{BadgerMecX Materials}},
year = {2026},
note = {Library v1.1.0, record glulam-gl32h},
url = {https://staging.badgermecx.com/materials/glulam-gl32h/}
}