Timber · Glued laminated timber, combined · orthotropic

GL32c

EN 14080:2013 · strength class

GL32c is a combined glued laminated timber class to EN 14080:2013. Its characteristic bending strength is 32 MPa. Along the fibres E₁ = 13.5 GPa; across them E₂ = 0.3 GPa.

Record
glulam-gl32c
Library
v1.1.0
Properties
15
Sources
1
Build check
passed ✓
Viewing as
guest
+ Compare Cite Download · PRO
E₁ · Modulus, direction 1 13.5GPa mean[1]
f_m,k · Bending strength 32MPa char[1]
f_t,0,k · Tension parallel to grain 19.5MPa char[1]
ρ · Density 440kg/m³ mean[1]

Elastic constants

orthotropic
SymbolPropertyValueUnitBasisRef.
E₁ Modulus, direction 1 ⓘ E_0,g,mean 13.5 GPa mean [1]
E₀,₀₅ Modulus parallel to grain, 5 % fractile 11.2 GPa char [1]
E₂ Modulus, direction 2 ⓘ E_90,g,mean 0.3 GPa mean [1]
E₃ Modulus, direction 3 ⓘ E_90,g,mean 0.3 GPa mean [1]
G₁₂ Shear modulus 1-2 ⓘ G_g,mean 0.65 GPa mean [1]
G₁₃ Shear modulus 1-3 ⓘ G_g,mean 0.65 GPa mean [1]
G₀₅ Shear modulus, 5 % fractile 0.54 GPa char [1]

Physical, thermal and electrical

at 20 °C
SymbolPropertyValueUnitBasisRef.
ρ Density 440 kg/m³ mean [1]
ρ_k Density, characteristic (5 % fractile) 400 kg/m³ char [1]

Strength

a band applies up to and including its upper limit
SymbolPropertyValueUnitBasisRef.
f_m,k Bending strength 32 MPa char [1]
f_t,0,k Tension parallel to grain 19.5 MPa char [1]
f_t,90,k Tension perpendicular to grain 0.5 MPa char [1]
f_c,90,k Compression perpendicular to grain 2.5 MPa char [1]
f_v,k Shear strength 3.5 MPa char [1]
f_c,0,k Compression parallel to grain 24.5 MPa char [1]

Notes

  • EN 338 and EN 14080 give no Poisson's ratios; a 3D analysis needs them from another source.

Sources

every value names one
  1. EN 14080:2013, Timber structures — Glued laminated timber, Tables 4 and 5Copies checked: 1, 2, 3, 4

min product standard minimum char characteristic design code value for design typical datasheet or textbook derived worked out here, formula shown

Cite this page

for reports and papers

BadgerMecX Materials (2026). GL32c — material properties, EN 14080:2013. Library v1.1.0, record glulam-gl32c. https://staging.badgermecx.com/materials/glulam-gl32c/ (accessed 2026-11-26).

@misc{badgermecx_glulamgl32c,
  title  = {GL32c -- material properties, EN 14080:2013},
  author = {{BadgerMecX Materials}},
  year   = {2026},
  note   = {Library v1.1.0, record glulam-gl32c},
  url    = {https://staging.badgermecx.com/materials/glulam-gl32c/}
}

Export and related