Steel · Stainless steel, duplex · isotropic
1.4362 (X2CrNiN23-4)
EN 1993-1-4 · EN 10088 · annealed (nominal design values) · also X2CrNiN23-4
1.4362 (X2CrNiN23-4) is a duplex stainless steel to EN 1993-1-4 · EN 10088. Its nominal yield strength is 400–450 MPa, depending on the product form and thickness. E = 200 GPa, ν = 0.3 and α = 13 × 10⁻⁶/K (design values).
- Record
- stainless-14362
- Library
- v1.1.0
- Properties
- 10
- Sources
- 2
- Build check
- passed ✓
- Viewing as
- guest
Elastic constants
isotropic| Symbol | Property | Value | Unit | Basis | Ref. |
|---|---|---|---|---|---|
| E | Young's modulus ⓘ EN 1993-1-4 2.1.3 | 200 | GPa | design | [1] |
| ν | Poisson's ratio | 0.3 | – | design | [1] |
| G | Shear modulus ⓘ G = E/(2(1 + ν)); SCI P413 rounds it to 76.9 GPa for 200 GPa | 76.92 | GPa | derived | [1] |
| K | Bulk modulus K = E / 3(1 − 2ν) | 166.7 | GPa | derived | — |
| λ_L | Lamé constant λ_L = Eν / (1 + ν)(1 − 2ν) | 115.4 | GPa | derived | — |
| c₀ | Bar wave speed c₀ = √(E/ρ) | 5064 | m/s | derived | — |
Physical, thermal and electrical
at 20 °C| Symbol | Property | Value | Unit | Basis | Ref. |
|---|---|---|---|---|---|
| ρ | Density ⓘ EN 10088-1 values as quoted by Outokumpu | 7800 | kg/m³ | typical | [2] |
| α | Coefficient of thermal expansion ⓘ mean, 20–100 °C | 13 | 10⁻⁶/K | typical | [2] |
| λ | Thermal conductivity ⓘ at 20 °C | 15 | W/(m·K) | typical | [2] |
| c_p | Specific heat capacity ⓘ at 20 °C | 500 | J/(kg·K) | typical | [2] |
| ρ_e | Electrical resistivity ⓘ at 20 °C | 0.8 | µΩ·m | typical | [2] |
| a | Thermal diffusivity a = λ / (ρ·c_p) | 3.846 | mm²/s | derived | — |
Strength
a band applies up to and including its upper limit| Property | Product form | Thickness | Value | Unit | Basis | Ref. |
|---|---|---|---|---|---|---|
| f_y | C — cold rolled strip | t ≤ 8 mm | 450 | MPa | nominal | [1] |
| f_y | H — hot rolled strip | t ≤ 13.50 mm | 400 | MPa | nominal | [1] |
| f_y | P — hot rolled plate | t ≤ 75 mm | 400 | MPa | nominal | [1] |
| f_y | B — bars, rods and sections | t ≤ 160 mm | 400 | MPa | nominal | [1] |
| f_u | C — cold rolled strip | t ≤ 8 mm | 650 | MPa | nominal | [1] |
| f_u | H — hot rolled strip | t ≤ 13.50 mm | 650 | MPa | nominal | [1] |
| f_u | P — hot rolled plate | t ≤ 75 mm | 630 | MPa | nominal | [1] |
| f_u | B — bars, rods and sections | t ≤ 160 mm | 600 | MPa | nominal | [1] |
Sources
every value names one- EN 1993-1-4:2006+A1:2015, Eurocode 3 — Stainless steels, Table 2.1 and 2.1.3Copies checked: 1, 2
- EN 10088-1, Stainless steels — List of stainless steels, physical properties (as quoted by Outokumpu datasheets)Copies checked: 1, 2, 3, 4
min product standard minimum char characteristic design code value for design typical datasheet or textbook derived worked out here, formula shown
Cite this page
for reports and papersBadgerMecX Materials (2026). 1.4362 (X2CrNiN23-4) — material properties, EN 1993-1-4 · EN 10088. Library v1.1.0, record stainless-14362. https://staging.badgermecx.com/materials/stainless-14362/ (accessed 2026-11-26).
@misc{badgermecx_stainless14362,
title = {1.4362 (X2CrNiN23-4) -- material properties, EN 1993-1-4 · EN 10088},
author = {{BadgerMecX Materials}},
year = {2026},
note = {Library v1.1.0, record stainless-14362},
url = {https://staging.badgermecx.com/materials/stainless-14362/}
}